NYC 9/11 Public Portal Document
Articles • Lioyetal.
We detected no differences between the The findings of skin cells was consistent widi construction debris (including cement, ver
exposed copper mirrors and the controls, the types of particles usually found in dust in miculite, plaster, synthetic foam, glass frag
indicating that these dust samples were not the indoor environment. ments, mineral wool fibers, paint particles,
corrosive toward base metals. This finding is Approximately 35% of the volume of the glass fibers, metals, calcite grains, and paper
consistent with the pH measurements. sample was in the form of loosely consoli fragments), quartz grains, low-temperature
Morphologic analyses. Detailed morpho dated clump.s of fibrous lint, of which the combustion material (including charred
logic analyses of each sample supported the greatest portion was glass fibers. An example woody fragments), and metal flakes. Wc esti
general characterizations presented in Table 1. of the typical form of the glass fibers is shown mated that chrysotile asbestos fibers com
Cortlandt Street sample. The Cortlandt in Figure 4. In many cases the width was = 1 prised < 1 % of the sample by volume. Much
Street sample was mainly composed of con pm (to > 10 pm), and the length ranged of the chrysotile asbestos had carbonate
struction debris [including vermiculite, plas from 5 to 100 pm. The fiber shown in Figure binder adhered to it. We observed some hair
ter, synthetic foam, glass fragments, paint 4 is not a “clean” glass fiber; other materials fibers and tarry fragments in the sample.
particles, glass fibers, lead (Figure 3), calcite are agglomerated along the rod. This is typi Approximately 10% of the volume of the
grains, and paper fragments], quartz grains, cal of features noted for many different types sample was in the form of loosely consoli
low-temperature combustion material of particles in each sample. The SEM analysis dated clumps of fibrous lint, of which the
(including charred woody fragments), and of the fraction <75 pm in diameter revealed greatest portion was glass fibers. The SEM
glass shards. Chrysotile asbestos fibers were marry glass fibers cud cement par ticles, sonre analysis of the fraction <75 pm in diameter
estimated to comprise < 1 % of the sample by in a fibrous form containing calcium, silicon, revealed many glass fibers and cement parti
volume, and much of the chrysotile adhered and sulfur, and some particles were com cles, some in a fibrous form, containing cal
to carbonate binder. Some skin cells and posed of calcium carbonate (Figure 5). cium, silicon, and sulfur.
dyed cotton fibers were present (.5,21-23). Chrysotile asbestos fibers, identified by We used SEM and TEM to examine
transmission electron microscopy (TRM), chrysotile asbesto.s fibers, lead paint frag
were found in the < 75-pm fraction. None ments, iron-chromium particles, and soot
of the analyzed particles contained lead, particles found in the < 75-pm fraction. The
chromium, cadmium, or mercury, although soot particles were in the submicron size
chromium and cadmium were quantified in range (Figure 6). No particles containing
this sample by ICP/MS analyses. cadmium (detected by ICP/MS) or mercury
Cherry Avenue sample. The Cherry were found at less than minimum detection
Avenue sample is mainly composed of limits in the 1,000 particles analyzed from
this sample.
Market Street sample. The Market
Street sample was also composed of con-
stiuction debris (including vermiculite, plas
ter, synthetic foam, glass fragments, paint
particles, mineral wool fibers, glass fibers,
calcite grains, and paper fragments), quartz
grains, low-temperature combustion material
(including charred woody fragments), and
Figure 3. Appearance of lead from the Cortlandt metal flakes. Chrysotile asbestos fibers made
Street sample. up < 1% of the sample by volume, and
much of the chrysotile adhered to carbonate
binder. This result is different from the bulk
Figure 5. Coarse calcium carbonate particle mass results, which indicated 3.0% asbestos;
detected in the Cortlandt Street sample. this indicates that the sample was not homo
geneous. Some dyed cotton fibers, tarry frag
ments, pollen grains, and metal flakes were
also present. Approximately 10% of the vol
IssssSitOisssi ume of the sample was in the form of loosely
coirsolidated clumps of fibrous lint, of which
the greatest portion was glass fibers, fhe
SEM analysis of the fraction <75 pm in
diameter revealed many glass fibers and
cement particles, some in a fibrous form
containing calcium, silicon, and sulfur.
Chrysotile asbestos fibers, identified by
TEM, were found in the fine fraction. We
foimd no particles containing lead, chromium,
cadmium, or mercury in the single particles
analyzed from the Market Street sample,
MVA4888 U8t7 ittiiitwi although all but mercury were detected by
MVA4S03 Lists Park 2-S the ICP/MS analyses.
Markel M 5 pm
Figure 6. A soot particle containing coagulated The morphologic differences between
Figure 4. Glass fiber detected in the Market Street ultra-fine particles detected in the Cherry Street each of the collected samples were minor
sample. sample. and could be attributed to the fact that we
708 VOLUME 1101 NUMBER 7 I July 2002 • Environmental Health Perspectives
CITY_21MC100_013389342
NYC-WTC_000436290
OCR can misread numbers and units. Confirm readings against the page image before using them.